Case Share:Thermal paper manufacturing troubleshoot and solution-Hunan Jiaqi New Materials Co., Ltd

News

Case Share:Thermal paper manufacturing troubleshoot and solution

Created on:2026-10-30 10:25

Case Share:Thermal paper manufacturing troubleshoot and solution

 

Problem Description from Client:

 

 

“if the thermal paper formula and paper quality were unchanged during production, what could be causing the thermal paper's quality to deteriorate and the durability of the print on the paper to decrease? Thermal paper may be of good quality during production, but after two days, the print quality on samples of the same paper deteriorates. Also, after two days, the print gradually disappears from the printed thermal paper. “

 

“When it was hot, we had a problem with the thermal paste constantly thickening and becoming more viscous. At the same time, the humidity was high.”

 

 

 

img1

Photo 1:print quality after production

 

img2

Photo 2:print quality after 2 days

 

 

thermal paper production details confirmation with cilent(base paper/formulation/equipment/QC) as per below table:

 

item

Jiaqi comments

Base paper specification

OK

Precoat slurry formulation

OK

Thermal sensitive coat slurry formulation

there are some minor issues with the formulation

Calender Information:

Material: polyurethane, hardness: 80 Shore A

The hardness of this calendering roller is too low,result in poor calendering effect.Fortunately, it is coated using two scrapers.

Particle size of slurry:no data

No testing machine to test the quality of thermal paper coating slurry

Thermal paper coating slurry production machine status:

 Two mills for each grinding machine;

 60 liter;

 Screen size:0.5mm

 Grinding balls is 125kg

 Grinding ball size:1.2-1.4mm

 Grinding time:4 hours

 grinding temperature:12-15 degrees Celsius

 grinding equipment and the grinding process are far from sufficient

should probably use a particle size analyzer to test the A and B materials separately.

The sieve and beads of the grinder are too coarse, which directly results in the particle size of the grinding liquid being unable to be small. At the same time, the amount of beads in the grinder is a bit low,based on such equipment parameters, it is unlikely to grind the coating properly in just 4 hours.

 

Short-term improvement measures:

 

 

1.try increasing the pre-coating weight to around 5 g/m², which should resolve or significantly improve the issue.

 

2.Based on the grinding machine parameters, the specifications for the screen and beads are too large, and the amount of beads loaded is also insufficient. extend the grinding time from 4 hours to 12 hours.

 

3.The separator with a sieve is best configured with two machines of 0.4mm paired with 0.8-1.0mm beads, and two machines of 0.3mm paired with 0.6-0.8mm beads. Each grinder should be loaded with 140-150 kilograms of beads.

 

Long term improvement measures:

 

1.       Purchase one particle size testing machine to test the quality of coating slurry.

2.       Optimize the coating slurry formulation

3.       Update the calendering roller in the thermal paper coating production line

 

 

 

 

News